some
Another month, another workshop with the Online Guild of Weavers, Spinners and Dyers, this time Medieval Dyeing with Deb Bamford. I've done a lot of natural dyeing over the last 30+ years, but never in a very systematic way, so I thought this workshop would be a good opportunity to get some tips for improvement and also try to be a bit more disciplined in recording my efforts.
We started several weeks before the workshop proper, by preparing copper and iron solutions to use as modifiers. I put rusty nails in one jar, and some copper wire in another, topped them up with half-and-half vinegar and water, put the lids on and left them in a sunny place.

The third modifier was ammonia - traditionally stale urine was used, but I decided that was taking it just a tad too far and bought a bottle of ammonia from the ironmonger!

The materials: I chose parts of two fleeces - a fine white crossbred fleece and some Shetland that I had already (rather unsucessfully) solar-dyed with an exhaust bath of Cutch waste to a pale beige. I also used some Blue-faced Leicester tops, silk hankies, degummed cocoons, broken silk tops and silk noil tops, cashmere/silk blend tops, a skein of lovely soft cashmere yarn (commercially spun) and  small skeins of handspun silk and wool yarns. Finally, I experimented with dyeing batts of drum-carded (washed) wool
 I prefer to dye fibre rather than yarn or fabric for several reasons: I'm a spinner and occasional weaver so I'm not particularly interested in dyeing commercially spun yarn or fabrics - although I do make some exceptions to this; if the results aren't good I havent wasted the effort of spinning/weaving; if the dye takes unevenly on yarn or fabric there's not a great deal you can do about it - on fibre the dye pretty much always takes unevenly but you can then choose whether to exploit that to get a subtle variegation in the yarn, or blend thoroughly before spinning to get more homogenous colours. And of course you can blend the fibre from two or more dyelots to improve the shade or get a more useful quantity.
So I was starting to deviate from the workshop instructions before really getting started as Deb had recommended using yarn or fabric - which certainly run less risk of felting. Also commercially prepared fibres, spun or un-spun, seem often to take up dye better - I guess that the commercial scouring methods leave the fibres more porous than even a thorough washing at home.

That brings us to the first stage of preparation. I had already washed the fleece pretty thoroughly using washing soda and hot water at least twice. The first set of instructions were about scouring - getting rid of any last traces of grease or dirt in the fibre. Using my late mothers jam pan (aluminium, but I was going to use alum mordant anyway), the batches of soaked fibre were gently heated and simmered with detergent:
The next stage was to mordant it. Mordanting helps the dye to attach to the fibre. Some mordants are very toxic but for this workshop we used alum, in small enough amounts that it should all have been absorbed on to the fibres. However it is important to always be really carefull!!

I kept the mordanted fibres wet, in large plastic boxes with lids, which is fine over a few days - any longer before dyeing and I would have dried them and then soaked them again before dyeing.

The first dyestuff was good old onion skins. because I've used this many times I thought I'd try it out on the pre-dyed Shetland wool. This dye is substantive, which means it doesn't need a mordant. I had been collecting the dry papery outer skins for a few weeks - they keep really well in a paper bag.
I used essentially the same method to extract  all the dyes: I put them in a pan and poured boiling water over them, then left them to soak overnight. the next day I boiled them for about an hour, and again left them to soak overnight. The onion skins were the only dye I didn't tie up in muslin, instead I strained them out of the dye liquor before I put the wet fibres in.

Again, roughly the same method for all the dyes - after removing the dyestuff and entering the wet fibres, I heated the dyebath very slowly to 80 degrees centigrade. This took about two hours. Then I kept it on  a very low heat, checking that it didn't go above 80, for an hour, before switching off the heat and leaving it to cool and steep for up to 24 hours.

The next stage was to take the fibre out and divide it into smaller batches to experiment with the different modifiers. I just split the onion-dyed fibre into two batches and rinsed one.

I added a few spoonfuls of the iron solution to the dye, until it changed colour, going much darker. Then I put the second batch of dyed wool back in and heated it gently for about 15 minutes (from cold). Then I rinsed and dried the fibre:
To keep track of all my samples I cut out tags from a plastic carton, and numbered them in waterproof marker pen. That way I could tie them on to the samples as soon as they came out of the dyebath, without them being spoiled by getting wet.

The next dyestuff was Weld. I followed the same extracting and dyeing methods, using wool that had been pre-mordanted with alum and cream of tartar. I then divided the wool into six batches and the dye liquor into three. These were modified as follows:
the first wool sample #3: no modifier
I added a couple of spoonfuls of ammonia to the first dye batch and put in one wool sample #4. heated gently for 10 minutes then rinsed and dried
I added a few spoonfulls of copper solution to the second dye batch, put in two wool samples and heated gently for 10 minutes then took out one #5 and rinsed and dried. added a couple of spoonfuls of ammonia, heated gently for 10 minutes then rinsed and dried the other sample #6
I did the same thing with the last dye sample but using iron solution instead of copper, giving me samples #7 (iron) and #8 (iron + ammonia)
You can see the dramatic effect of ammonia on the samples on the right. The water here in Perthshire may be quite acidic, the alkali really brings out the colour. Copper had less effect than expected - perhaps the solution wasn't very strong, but iron darkened and 'saddened' the colour.

Next up was Dyers Broom, using the same methods as for Weld, and with very similar results:
The samples without ammonia are all a bit disappointing so I will keep a tiny amount of each as a record and then put them all in a dilute solution of ammonia to bring out the yellows. Actually yellow is a colour I rarely use so once I have spun them I may well over-dye them with indigo to try for some greens - it will be interesting to see if the ammonia has an effect on that.

So with the yellow/greens out of the way it was time to move on to (for me) the more interesting dyestuffs: brazilwood and madder.  However I wanted to dye more fibre in the 'exhaust' dyebaths with these two so all the modifications were done with the modifiers diluted in warm water rather than in the dye liquor. Using otherwise the same basic methods and modifiers I got these colours from Brazilwood:
The transformation from peachy oranges to purples with the ammonia was almost instant and really dramatic The tips of the fibres had as always taken up more dye and with ammonia they went bright red against magenta, with iron and ammonia they were almost navy blue against purple.
 Silk did not seem to dye as well as wool with brazilwood:


For each of the 'exhaust' baths I re-boiled the muslin bag of dyestuff in the original dye liquor for an hour or two, then left it to steep for at least 24 hours.

the second Brazilwood bath gave these:
Top right: BFL tops, bottom; silk cocoons, both modified with a small amount of ammonia
Top left: fine crossbred fleece, modified with iron and then ammonia

A third 'exhaust' on drum-carded wool modified with iron and ammonia gave this blue

Madder was next, on fibres mordanted with alum but no cream of tartar as this is supposed to give better colours. Using the same methods as brazilwood gave:
There is a bit of silk top attached to #26 - no modifier The silk has taken up the colour well in places but is quite patchy. I also dyed some yarn samples and silk  in this dye bath, which were also a bit uneven.

In the second madder dyebath I dyed two batts of carded wool  which came out a good strong slightly brickish red, very even. Then I transferred the dye to an old copper pan and dyed the third batch, more carded wool, in it. I left it to steep overnight without stirring after the heating phase, and the final shade of the batt was quite varied, as some parts were touching the copper and some were not.

The pan had been quite tarnished (i think it has been in my garden shed for about 15 years!!) but after the dyeing the parts under the water level were much brighter so ther had clearly been some kind of reaction.

Even though I had only started with 100g each of brazilwood and madder, there still seemed to be a lot of colour left after three dyebaths, so I transferred the liquor and bags of dyestuff to large jars, added alum and fibre, for solar dyeing. They will sit on my windowsill for several months but already the fibres look as if they have taken up plenty of colour. I also set up a solar jar with un-used madder, for comparison - it s the biggest one, on the right.

As if I didn't have enough different dyes and modifications to try out, I also experimented with soome dried Hibiscus flowers from Turkey
These were actually sold for making a drink, mixed with cloves and chunks of ginger root and cinnamon bark. I picked out most of the spices but the simmering dyepot, and even the dyed fibre, had a subtle spicy aroma! In the first dyebath I dyed 50g of cashmere yarn and 50g of silk hankies
Not the rich ruby red of the dye liquor, but a very pretty shade, quite pink in some lights but more beige in others. The second dyebath gave a paler more beige shade on silk. All were pre-mordanted with alum and cream of tartar. I tried modifying tiny samples with both ammonia and vinegar but both seemed to make the colour less pink.

All together I dyed 44 samples over three very enjoyable weeks. I will probably leave the yellow/green dyes for those who appreciate those colors more than I do, but the range of pinks, reds and purples that I got has whetted my appetite for more dyeing. I have sown a tray of japanese indigo seeds in my greenhouse so hopefully by the end of the summer I will have enough to attempt some blues!! In the meantime I will enjoy spinning with colour for the next few weeks....